Applicable to fully processed and PP grade Products coated with C6W Coating. |
| Welding parameters |
| 1 |
Punching Oil on Lamination |
The Laminations should be thoroughly cleaned to
remove punching oil for better results |
| 2 |
Burr on Edges µm |
< Than 30 microns |
| 3 |
Type of Welding |
Plasma TIG Welding |
| 4 |
Shielding Gas |
Argon (99.9 % Purity) |
| 5 |
Argon Gas Flow |
4-5 Lit/Min |
| 6 |
Electrode Dia |
1.6 mm |
| 7 |
Gap Between Electrode and Material |
1.8 - 3.2 mm |
| 8 |
Clamping Pressure |
5 Kg/cm,min. |
| 9 |
Welding Current |
18 - 24 Amps |
| 10 |
Torch Speed |
30 - 35cm/Min |
|
|
|
|
|
|
|